Hardwood · Asia
Indian rosewood: hardness, strength and shrinkage
Indian rosewood has a Janka hardness of 3,170 lbf, stiffness of 1.78 million psi and bending strength of 16,900 psi (USDA Wood Handbook). It weighs about 52.4 lb per cubic foot at 12% moisture and shrinks 5.8% across the growth rings from green to dry.
- Janka hardness
- 3,170 lbf 6th of 168
- Stiffness (E)
- 1.78 million psi 72nd of 184
- Bending strength
- 16,900 psi 44th of 184
- Crushing strength
- 9,220 psi
- Specific gravity
- 0.75 17th of 183
- Weight at 12%
- 52.4 lb/ft³ 4.37 lb per board foot
- Shrinkage, green to dry
- 5.8% across rings 2.7% along them
Check a shelf in indian rosewoodHow much does it move?Compare all 184 woods
How it compares
At 3,170 lbf, indian rosewood is a very hard wood: 233% as hard as white oak (1,360 lbf), and 6th of 168 for hardness among the woods that were Janka tested. Under about 700 lbf a floor or tabletop dents from a dropped fork; above 1,200 it takes everyday knocks.
Its stiffness of 1.78 million psi is 72nd of 184, and white oak's is 1.78. Stiffness, not strength, decides how far a shelf or rail bends under a load; strength decides when it breaks. Its bending strength is 16,900 psi, 111% of white oak's.
Will a shelf of it sag?
A 3/4-inch shelf, 11 1/4 inches deep (a 1×12), carrying 20 pounds per foot, stays under the 1/600 "looks bent" limit after several years for spans up to about 31" in indian rosewood. Longer than that and it will visibly bow; thicker stock, a front edge strip or a middle support fixes it. Estimated Worked out from the Handbook's stiffness with the creep allowance used in the shelf sag calculator; it is a woodworker's rule of thumb, not a structural check.
How much it moves
Across the growth rings (plainsawn faces) it shrinks 5.8% from green to oven dry; along them (quartersawn faces) 2.7%; in volume 8.5%. Between a dry winter room (30% humidity, about 6.2% moisture) and a humid summer one (60%, about 11.0%) a 12-inch plainsawn board changes width by about 0.12 inch, and a quartersawn one by about 0.05 inch. Try your own width and humidity.
Weight
At 12% moisture it weighs about 52.4 pounds per cubic foot, or 4.37 pounds per board foot. A 1×6 board 8 feet long (4 board feet) comes to roughly 17.5 pounds. Green lumber weighs more, because the water has not dried out.