Pacific silver fir has a Janka hardness of 430 lbf, stiffness of 1.76 million psi and bending strength of 11,000 psi (USDA Wood Handbook). It weighs about 30.1 lb per cubic foot at 12% moisture and shrinks 9.2% across the growth rings from green to dry.
- Janka hardness
- 430 lbf 150th of 168
- Stiffness (E)
- 1.76 million psi 77th of 184
- Bending strength
- 11,000 psi 121st of 184
- Crushing strength
- 6,410 psi
- Specific gravity
- 0.43 133rd of 183
- Weight at 12%
- 30.1 lb/ft³ 2.51 lb per board foot
- Shrinkage, green to dry
- 9.2% across rings 4.4% along them
Check a shelf in pacific silver firHow much does it move?Compare all 184 woods
How it compares
At 430 lbf, pacific silver fir is a soft wood: 32% as hard as white oak (1,360 lbf), and 150th of 168 for hardness among the woods that were Janka tested. Under about 700 lbf a floor or tabletop dents from a dropped fork; above 1,200 it takes everyday knocks.
Its stiffness of 1.76 million psi is 77th of 184, and white oak's is 1.78. Stiffness, not strength, decides how far a shelf or rail bends under a load; strength decides when it breaks. Its bending strength is 11,000 psi, 72% of white oak's.
Will a shelf of it sag?
A 3/4-inch shelf, 11 1/4 inches deep (a 1×12), carrying 20 pounds per foot, stays under the 1/600 "looks bent" limit after several years for spans up to about 31" in pacific silver fir. Longer than that and it will visibly bow; thicker stock, a front edge strip or a middle support fixes it. Estimated Worked out from the Handbook's stiffness with the creep allowance used in the shelf sag calculator; it is a woodworker's rule of thumb, not a structural check.
How much it moves
Across the growth rings (plainsawn faces) it shrinks 9.2% from green to oven dry; along them (quartersawn faces) 4.4%; in volume 13%. Between a dry winter room (30% humidity, about 6.2% moisture) and a humid summer one (60%, about 11.0%) a 12-inch plainsawn board changes width by about 0.19 inch, and a quartersawn one by about 0.09 inch. Try your own width and humidity.
Weight
At 12% moisture it weighs about 30.1 pounds per cubic foot, or 2.51 pounds per board foot. A 1×6 board 8 feet long (4 board feet) comes to roughly 10.0 pounds. Green lumber weighs more, because the water has not dried out.