Hardwood · North America
Sassafras: hardness, strength and shrinkage
Sassafras is a hardwood, stiffness of 1.12 million psi and bending strength of 9,000 psi (USDA Wood Handbook). It weighs about 32.2 lb per cubic foot at 12% moisture and shrinks 6.2% across the growth rings from green to dry.
- Janka hardness
- not tested
- Stiffness (E)
- 1.12 million psi 168th of 184
- Bending strength
- 9,000 psi 156th of 184
- Crushing strength
- 4,760 psi
- Specific gravity
- 0.46 124th of 183
- Weight at 12%
- 32.2 lb/ft³ 2.68 lb per board foot
- Shrinkage, green to dry
- 6.2% across rings 4% along them
Check a shelf in sassafrasHow much does it move?Compare all 184 woods
How it compares
The Wood Handbook gives no Janka hardness for sassafras, so compare it by density instead: a specific gravity of 0.46 is 124th of 183.
Its stiffness of 1.12 million psi is 168th of 184, and white oak's is 1.78. Stiffness, not strength, decides how far a shelf or rail bends under a load; strength decides when it breaks. Its bending strength is 9,000 psi, 59% of white oak's.
Will a shelf of it sag?
A 3/4-inch shelf, 11 1/4 inches deep (a 1×12), carrying 20 pounds per foot, stays under the 1/600 "looks bent" limit after several years for spans up to about 27" in sassafras. Longer than that and it will visibly bow; thicker stock, a front edge strip or a middle support fixes it. Estimated Worked out from the Handbook's stiffness with the creep allowance used in the shelf sag calculator; it is a woodworker's rule of thumb, not a structural check.
How much it moves
Across the growth rings (plainsawn faces) it shrinks 6.2% from green to oven dry; along them (quartersawn faces) 4%; in volume 10.3%. Between a dry winter room (30% humidity, about 6.2% moisture) and a humid summer one (60%, about 11.0%) a 12-inch plainsawn board changes width by about 0.13 inch, and a quartersawn one by about 0.08 inch. Try your own width and humidity.
Weight
At 12% moisture it weighs about 32.2 pounds per cubic foot, or 2.68 pounds per board foot. A 1×6 board 8 feet long (4 board feet) comes to roughly 10.7 pounds. Green lumber weighs more, because the water has not dried out.